> On Sun, Jul 03, 2016 at 12:33:04PM +0200, Andrea Baldoni wrote:
>> Hello.
>> I repeated the experiment with a better setup, I also added
>> some alloys that are already arrived. So far, a really "low"
>> EMF solder hasn't been identified.
>
>> Measurements have been done between water ice point and boiling
>> point with Agilent 34401A. I don't expect the curves be linear,
>> but here it's assumed they are.
>
>> Copper - Sn96.5/Ag3/Cu0.5 -> 3.35uV/K
>> Copper - Sn95.5/Ag3.8/Cu0.7 -> 3.22uV/K
>> Copper - Sn60/Pb40 -> 3.34uV/K
>> Copper - Pb92.5/Sn5/Ag2.5 -> 3.02uV/K
>
>> Copper - Brass -> 3.30uV/K
>
>> I am waiting for Sn96/Ag4, Sn99/Cu1.
>
> Any plans on testing Sn42/Bi57.6/Ag0.4 ?
>
> Thanks,
> Herbert
>

It would also be interesting to get SN100C in the mix if you can find it...